Residue-Free Labels Latest in Tools and Supplies

Natural Pore Filler for a Tung Oil Finish

A finisher gets suggestions for filling pores on Walnut stool tops before applying Tung oil. July 3, 2008

Question
Is there an ideal pore filler for a tung oil finish? Is there a green pore filler? I'm doing tests for some walnut stools for a restaurant and I want an easy to repair and dark finish for it. I've had luck with pigmented wax, but will that migrate onto clients clothing?

Forum Responses
(Finishing Forum)
From contributor D:
How much experience do you have with water or chemical dyes? If you feel comfortable with them then I suggest you use potassium permanganate to dye your pieces with, then apply a thin coat of tung, let it dry, then apply a linseed oil base grain filler - the old kind not the new fast dry type. After that has thoroughly dried apply as many coats of the poly tung as you desire for build - usually three is sufficient. This way no color is on the surface of the wood. The pores will be filled well and the finish will still be quite repairable with the PP and tung as you go



From the original questioner:
I've used a variety of chemical and water dyes, but not that one. Do you have a good source for it? Same with the grain filler: what brand is the type you suggest and where should I buy it? Can I make my own?


From contributor C:
If you have a fairly local Culligan water softener dealer you can get it there for about $25.00 in a container. I know someone still makes the LO filler but I don’t know it off-hand. Don’t exceed 4 oz. per gallon of the PP. Start with 1 oz. per gallon. Make up just what you think you'll need. It loses its potency after a short while.


From contributor R:
Jasco makes what they call a natural wood filler but it’s kind of a yellowish/tan color. From my experience you can add oil colors to it as well as dry powders.

Wood-Kote out of Oregon makes a paste wood filler that’s as white as typing paper and you can add colors to it as well. UTC or artist oils or the powdered dye colors work pretty well, just stay away from the water soluble ones because you can mix it up until the stars fall from the sky and they still won’t dissolve.



From contributor C:
Contributor R - is Jasco the old type linseed oil base filler? This is what will be needed - and for his use oil colors would be best.


From contributor R:
Yes the Jasco formula is of a linseed oil base as is the paste wood filler from Wood-Kote. The only difference between the two is the color. As far as the color it’s up to the user. If you went with the powders you might want to mix them up first in some Naptha and then add the mixture into the filler. The oils seem to mix up rather easy into either of the two fillers.


From the original questioner:
Just an update: after trying out Wood-Kote, the fact that it left the surface looking glossy made me a little nervous about the compatibility with the Tung finish. It seems that the test I liked the best was with Rockler's Wonderfil, which sort of surprised me. It filled well enough for my purposes in one coat, smells like nothing, sanded and cleaned up easily, and looked great with an oil finish! One application before sealing the wood was enough for the job. Unless someone can come up with a reason why this is unwise, I think I have a winner.


AI enhanced answer (added Jan 27, 2025):

For filling pores on walnut before applying a Tung oil finish, consider these steps:

1. Sanding: Start with 150-grit sandpaper, progressing to 220-grit for a smooth surface. This helps in opening the pores slightly for better filler adhesion.

2. Pore Filler: Use a water-based or oil-based pore filler. For walnut, an oil-based filler like Zinsser's SealCoat or a commercial wood pore filler can work well. Apply the filler with a plastic scraper or a squeegee, working it into the pores.

3. Application: Spread the filler across the wood, ensuring it gets into the pores. Let it sit for a few minutes, then remove the excess with a rag or a card scraper, scraping diagonally to the grain to avoid pulling filler out of the pores.

4. Drying: Allow the filler to dry as per the manufacturer's instructions, usually several hours or overnight.

5. Sanding Again: Once dry, lightly sand with 320-grit sandpaper to remove any filler residue on the surface, leaving the filler only in the pores.

6. Seal: Before applying Tung oil, consider sealing the wood with a light coat of shellac or a sanding sealer to prevent the oil from darkening the filler too much.

7. Tung Oil: Apply Tung oil as usual, allowing it to penetrate the wood. The filled pores will give a more uniform appearance when the oil is applied.

Remember, the goal is to fill the pores without altering the natural beauty of the walnut. Keep the filler color close to walnut or slightly lighter to avoid a stark contrast.