Question
I am using a Holz-Her edge bander with Doris-25 adhesive cartridges to apply plastic laminate strips to IPB underlayment. I'm not getting good adhesion on the laminate. Any suggestions?

Forum Responses
(Laminate and Solid Surfacing Forum)
From Contributor O:
Are you priming the laminate? We have found that to be a necessity.



From the original questioner:
What do you use? Jowat water base primer has been suggested.


From Contributor B:
We spray the backside of the laminate with solvent based contact cement and let it dry before sending it through the edgebander. It works well for us.


From the original questioner:
Thanks everyone. I'm using the spray for the laminate first and it really works. I will try the Doris next time as it saves another step.